Hostname: page-component-586b7cd67f-l7hp2 Total loading time: 0 Render date: 2024-11-29T07:40:39.189Z Has data issue: false hasContentIssue false

Nano-Particulate of Aluminum Nitride Prepared by Pulsed Wire Discharge

Published online by Cambridge University Press:  17 March 2011

Yoshiaki Kinemuchi
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Channarong Sangurai
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Tsuneo Suzuki
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Hisayuki Suematsu
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Weihua Jiang
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Kiyoshi Yatsui
Affiliation:
Extreme Energy-Density Research Institute, Nagaoka University of Technology, Nagaoka, Niigata, 940-2188, Japan
Get access

Abstract

Nanoparticulates of aluminum nitride (AlN) have been synthesized by novel dry process, namely pulsed wire discharge where aluminum wire is exploded by an intense pulsed current (10-20 kA at the peak, half cycle of 10 μs) in NH3/N2 gas. The average size of the nanoparticulates was found to be 28 nm. Furthermore, narrow particle distribution of the particulates was observed, where geometric standard deviation was 1.29. Increasing charging energy enhances the nitridation of aluminum. The maximum content of AlN in synthesized particulates was ∼95 %. The sintered body with 80 % of density has been obtained by sintering at 1, 600°C for one hour.

Type
Research Article
Copyright
Copyright © Materials Research Society 2002

Access options

Get access to the full version of this content by using one of the access options below. (Log in options will check for institutional or personal access. Content may require purchase if you do not have access.)

References

1. Lan, Y. C., Chen, X. L., Cao, Y. G., Xu, Y. P., Xun, L. D., Xu, T. and Liang, J. K., J. Crystal Growth, 207, 247 (1999).Google Scholar
2. Cao, Y. G., Chen, X. L., Lan, Y. C., Li, J. Y., Xu, Y. P., Xu, T., Liu, Q. L. and Liang, J. K., J. Crystal Growth, 213, 198 (2000).Google Scholar
3. Jiang, W. and Yatsui, K., IEEE Trans. Plasma Sci., 26, 1498 (1998).Google Scholar
4. Suzuki, T., Keawchai, K., Jiang, W. and Yatsui, K., Jpn. J. Appl. Phys., 40 Pt.1 (2B), 1073 (2001).Google Scholar
5. Kotov, Y. A., Azarkevech, E. I., Beketov, I. V., Demina, T. M., Murzakaev, A. M. and Samatov, O. M., Key Engineering Mater., 132–136, 173 (1997).Google Scholar
6. Moura, F. J. and Munz, R. J., J. Am. Ceram. Soc., 80, 2425 (1997).Google Scholar
7. Grigoriu, C., Hirai, M., Nishiura, K., Jiang, W. and Yatsui, K., J. Am. Ceram. Soc., 83, 2631 (2000).Google Scholar
8. Komeya, K. and Inoue, H., J. Mat. Sci., 4, 1045 (1969).Google Scholar