238Pu-substituted zirconolite (CaPuTi2O7) was held at ≈350 K for a time sufficient to allow self-irradiation damage to convert the material to the metamict condition. Samples were then stored at 875 K, while dimensional and microstructural changes were monitored by dilatometry and transmission electron microscopy. Densification proceeded sporadically over a period of ≈400 days, attaining a final value of 4 vol% as a result of crystallization. The material was found to be friable at an intermediate stage of recovery, apparently as a result of internal strains. Evidence is presented that CaPuTi2O7 can exist in more than one metamict state, depending on extent of prior damage and thermal history.