EBSD Study of Indian Wootz Steel Artifacts to Infer Thermomechanical History by Observation of Carbide Distribution and Orientation

Published online by Cambridge University Press:  12 March 2010

A. Sullivan
Affiliation:
Centre for Material and Fibre Innovation, Deakin University, Geelong, Australia, 3217. E-mail: [email protected]
M. Barnett
Affiliation:
Centre for Material and Fibre Innovation, Deakin University, Geelong, Australia, 3217

Extract

Wootz is the name given to a crucible steel prepared in India. Coze noted that the name “wootz” first appeared in printed form in a report by Pearson in 1795. However, the origin of the name itself is unclear though it was proposed by Yule and Burnell in the Hobson-Jobson Dictionary that the word “wootz” could come from “ukku” in the Kanadda language.

Type
Materials Applications
Copyright
Copyright © Microscopy Society of America 2010

Introduction

Wootz is the name given to a crucible steel prepared in India. Coze [Reference Coze1] noted that the name “wootz” first appeared in printed form in a report by Pearson in 1795 [Reference Pearson2]. However, the origin of the name itself is unclear though it was proposed by Yule and Burnell in the Hobson-Jobson Dictionary [Reference Yule and Hobson-Jobson3] that the word “wootz” could come from “ukku” in the Kanadda language.

The historical impact and subsequent fame of wootz weaponry in the ancient world has created interest in what has come to be seen as an advanced material even by modern standards [Reference Srinivasan and Ranganathan4]. Ancient wootz artifacts are classed as high carbon (hypereutectoid) crucible steels and are characterized by high strength, hardness, and wear resistance [Reference Perttula5], but especially by their attractive surface pattern.

The ingots used to make wootz implements known to have been cast from as early as 300 BC, continuing into the 1700s, at which time the casting and forging knowledge declined and was eventually lost. No detailed written records exist of the forging methods used to make weapons and implements from cast wootz ingots [Reference Sherby6], leading to numerous duplication methods. Recent attempts have ranged from good approximations to almost identical reproductions [Reference Verhoeven, Pendray and Dauksch7, Reference Taleff8, Reference Perttula9, Reference Pendray10]. Notably absent from historical accounts are details of forging temperature, cooling rates, and the strains imparted at each forging step. This has prevented modern attempts to “rediscover” the ancient blacksmiths' method in which hot shortness during forging and duplication of the surface pattern are known obstacles.

Hot shortness causes the ingot to crack during forming and results from softening and melting of the pro-eutectoid cementite on prior austenite grain boundaries while working at white heat. This problem has largely been solved by forging at temperatures slightly above the A1 temperature (say ~750°C), thus enabling controlled breakage and spherodisation of the proeutectoid cementite (see Figure 1).

Figure 1: The iron-carbon phase diagram showing Wootz as a hypereutectoid steel with carbon content 1.6%, forged from cast ingot at high temperature using multiple cycles.

Duplication of the surface pattern has been more difficult and the mechanism by which it forms has been contested by a number of researchers [Reference Verhoeven, Pendray and Dauksch7, Reference Taleff8, Reference Verhoeven11, Reference Wadsworth12, Reference Verhoeven13, Reference Verhoeven14]. The materials and methods used to produce and forge wootz ingots directly affect whether or not a pattern can be produced. It is generally agreed that for artifacts having hypereutectoid compositions, the surface pattern results from a banded distribution of proeutectoid carbides alongside eutectoid carbides in a ferrite matrix formed during multiple forging cycles.

Other studies have shown the importance of characterizing the various carbide forms because they are useful in determining deformation and metallurgical history [Reference Barnett and Balasubramaniam15, Reference Verhoeven11, Reference Peterson16]. The extent and pattern of deformation is indicated by banding, cracking, and crystal orientation in the coarser, blocky type cementite [Reference Kumar17]. Metallurgical changes during forging are indicated by the morphology and crystal orientation of grain boundary (Widmanstatten and/or proeutectoid) and fine spheroidal cementite (spherodized pearlite and/or divorced eutectic) [Reference Verhoeven13, Reference Sullivan, Barnett and Balasubramaniam18, Reference Kumar17].

Two notable theories have been forwarded by Sherby and Wadsworth and by Verhoeven and Pendray to explain the origin of the proeutectoid carbides in forged wootz steel artifacts. Sherby and Wadsworth used a method of thermomechanical treatment employing hot and warm rolling to process pieces of hypereutectoid steels within a narrow temperature range [Reference Taleff8]. Such tightly controlled temperature during processing means their experiments are precise and reproducible, but the applicability of the work to genuine wootz microstructures has been questioned [Reference Verhoeven14]. The microstructures resulting from this method contain carbide patterns similar to ancient artifacts made from crucible steel, but there are notable differences. One significant difference is that all of the visible banding is in line with the direction in which the steel was rolled. Wadsworth and Sherby claim that this is simply an artifact of the production method, but no further processing has been carried out to prove their method could produce the appropriate banding if it were forged [Reference Jeffery19]. Verhoeven and Pendray proposed that the formation of the pattern is due to the alignment of spherodised cementite in the interdendritic zones where impurities accumulate during solidification. They determined that elements such as vanadium and molybdenum, even in quantities as low as 0.003 percent, promote the alignment of cementite at interdendritic zones through a selective ripening process [Reference Verhoeven11]. Other elements, which also promote banding, are chromium, niobium, and manganese [Reference Verhoeven, Pendray and Dauksch7]. Furthermore they showed that the banding behavior disappears and reappears with repeated thermal cycling [Reference Verhoeven13].

Debate over the origin and development of coarse carbide bands in wootz steel continues, and new methods of analysis offer alternative ways of interpreting these complex microstructures. Where previous work has relied mainly on light microscopy to learn about the metallurgical structures involved, the use of electron back scatter diffraction (EBSD) in the study of wootz steel is a new method in this field, with recent precedents in work done by Barnett and Balasubramaniam [Reference Barnett and Balasubramaniam15, Reference Sullivan, Barnett and Balasubramaniam18]. Unlike light microscopy investigations that can inspect artifact surfaces in their as-received condition, EBSD is destructive because the surface being analyzed must be finely polished. The advantage of data obtained by EBSD is that it contains unique information about the alignment of the crystal lattice, including metal grain and precipitate orientations and also phase distributions.

This study uses EBSD to investigate and identify relationships between carbide microstructure and thermomechanical history by collecting Euler angle data from crystal unit cells in polished wootz steel sections.

Compared to the more famous Damascus weaponry, traditional Indian weapons and implements made from wootz steel are less studied. This research summary presents an EBSD characterization of three Telangana artifacts from southern India, as identified in Table 1; two swords and one toddy tapper tool.

Table 1: Wootz artifact descriptions. Note that all items are hypereutectoid steels.

* Glow discharge optical spectrometry

Electron Backscatter Diffraction (EBSD)

When an electron beam is incident on a tilted crystalline sample, electron backscatter diffraction patterns are generated through an interaction with a small volume of the material (~20–50 nm in diameter) (see Figure 2a). In the present studies, EBSD data were collected on a Leo 1530 field-emission SEM, using an HKL Nordlys detector.

Figure 2: (a) Electron Backscatter Diffraction (EBSD) system schematic, (b) Kikuchi pattern [Reference Randle and Engler20].

The mechanism by which the diffraction patterns are formed can be described by the following principal features. The atoms in the material inelastically scatter a fraction of the electrons with only a small loss of energy to form a divergent source of electrons close to the surface of the sample. Some of these electrons are incident on atomic planes at angles that satisfy the Bragg equation (nλ = 2d sin θ), where n is an integer, λ is the wavelength of the electrons, d is the spacing of the diffracting plane, and θ is the angle of incidence of the electrons on the diffracting plane. These electrons are diffracted to form a set of paired large-angle cones (Kossel cones) corresponding to each diffracting plane. When used to form an image on the fluorescent screen, the regions of enhanced electron intensity between the cones produce the characteristic Kikuchi bands of the electron backscatter diffraction pattern (see Figure 2b).

The center line of each Kikuchi band corresponds to the intersection with the phosphor screen of the diffracting plane responsible for the band. The Kikuchi bands as a group are characteristic of the single crystal's structure and orientation. The angular position of the Kikuchi bands can be found automatically with a Hough transform [Reference Randle and Engler20] and used in conjunction with a crystallographic database to calculate the crystal orientation of the sample region that formed the pattern.

The measured crystal orientations are displayed in Euler angle maps and in pole figures. Euler angles are used to describe crystallite orientations within a specimen. This involves specific rotations that transform the sample coordinate system into the crystal coordinate system and vice versa. The Bunge convention [Reference Bunge21] is most commonly used in metallurgy (see Figure 3).

Figure 3: The three Euler angles: (ϕ1, Φ, ϕ2) represent the following (ordered) set of rotations, which are defined here. (1) A rotation of ϕ1 about the z-axis followed by, (2) a rotation of Φ about the rotated x-axis (u) followed by, (3) a rotation of ϕ2 about the rotated z-axis (z′).

Pole figures are stereographic projections for chosen crystal directions. An example of a pole figure construction for a simple cubic crystal is shown in Figure 4. When a single grain is orientated in a particular manner relative to the specimen, the ⟨100⟩ normals to the cube planes project onto a sphere as shown in Figure 4a. A plane parallel to the specimen surface and passing through the center of the sphere intersects the sphere as a circle. The points where the ⟨100⟩ normals touch the sphere are then joined to the sphere's opposite pole (South Pole for points in the upper hemisphere. The stereographic projection (pole figure) is the shaded equatorial plane containing the poles 1′, 2′, and 3′ in Figure 4a. This process converts three-dimensional crystallographic directions into a set of two-dimensional points (Figure 4b). Only the upper hemisphere points are shown. This is repeated for the orientations of other grains in the sample to produce a pole figure that shows the distribution of that particular set of planes. If there is a tendency for the points to be arranged in a particular manner then this is called a texture. Furthermore, these data points are usually contoured to reflect the density or strength of any textures that may be present. The mean uniform density or MUD value in a pole figure shows the strength of the clustering of data relative to that from a random distribution.

Figure 4: (a) ⟨100⟩ pole figure construction depicting the cubic unit cell at an arbitrary orientation relative to the sample. The sample surface is parallel to the equatorial plane. (b) The resulting pole figure (stereographic projection of the poles 1, 2, and 3).

All EBSD data presented in this article have undergone a two-step noise reduction procedure to clean the maps at pixels where no or very poor quality EBSD patterns are generated because of grain boundaries, cracks, dislocation clusters, voids, inclusions, or around regions of damage on the sample surface. The first step of noise reduction involves the replacement of pixels having an orientation different from all neighbors (“lonelies”) with Euler angles of the dominant surrounding orientation. The second step involves filling non-indexed pixels (zero solutions) with Euler angles that are interpolations of the neighboring pixels. This has been applied in stages beginning with eight-neighbor pixels (conservative) and progressively decreasing the number of neighbors to one, until no un-indexed pixels remain in the map. Noise reduction has been applied equally to both the ferrite and cementite phases. Noise reduction is performed on the Euler data so that sub-grain orientation gradients are more readily observed in the cementite. Pole figures are relatively unaffected by this process.

Results

Three different Indian artifacts were analyzed by EBSD to characterize the carbide population. Sampling locations are identified in Figure 5. Carbide breakage is evident as voids in the microstructure that produce no data, and crystallographic alignment is displayed in pole figures. Low-angle boundaries within individual carbide particles are displayed as an overlay on low-magnification Euler angle maps of the carbide phase. Breakage and rotation are indicated by orientation clustering and rotation. Crystallographic orientation, spatial distribution, and/or ripening are displayed in high-magnification Euler angle maps of the fine carbide phase. This study presents orientation clustering data for coarse and fine carbides for each wootz artifact.

Figure 5: EBSD mapping regions indicated in red on the schematics for each artifact: (a) toddy tapper and (b) blades 1 and 2 with z ∥ [010] axis. The dotted lines in (b) show where inhomogeneous material was removed prior to analysis.

Two types of orientation clustering of the carbides were observed in the swords and to a lesser extent in the toddy tapper tool: (a) a micron-scale clustering within the coarse carbide bands with band spacing ranging from 30–100 μm and (b) a fine micron to sub-micron scale clustering of spheroidal particles, closely associated with proeutectoid cementite lying along prior austenite grain boundaries.

It is proposed that coarse carbide bands and fine carbide dispersions retain useful information about the forging method used to manufacture wootz artifacts. The proposed forging direction is indicated by carbide breakage and crystallographic alignment in the coarse carbide population. The impact of forging strain on the microstructure is indicated by the presence of low Euler angle boundaries and by the extent of breakage and rotation of coarse carbide particles. Forging temperature effects are indicated by the crystallographic orientation, spatial distribution, and/or ripening of fine carbides.

Coarse Carbide. Orientation clustering behavior in the carbide particles is detected by inspecting EBSD maps set to display Euler angles on a color scale. For each case, particles having the same or similar Euler angle color are identified as a group. Within each group of particles a single fragment is selected as a reference, approximately near the center of the cluster (in orientation space), and a gray scale assigned ranging from black to white, where black represents the reference orientation and white represents a deviation of 20º (Figure 6c, Figure 7c, Figure 8c). Although a 20º deviation of Euler angle was chosen arbitrarily, it is based on the assumption that if fragmentation of a single carbide particle occurs, the resulting fragments will rotate away from the starting orientation as the particles are worked into bands. The amount of rotation is expected to be proportional to the amount of strain imparted during forging. The objective is to test the concept that carbide banding is at least in part the result of fragmentation and subsequent alignment of as-cast coarse carbides in response to forging hammer blows. Forging impacts are known to be repeatedly applied to a cylindrical casting in order to produce a blade, thus forcing carbides to break and move by a combination of translation and rotation into sheets within the ferrite matrix.

Figure 6: Sword 1 EBSD data. (a) Large area map showing carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is vertical in all images. (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase based on 347 × 241 μm mapping area.

Figure 7: Sword 2 EBSD map. (a) Large area map showing carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is vertical in all images. (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase, based on 347 × 259 μm mapping area.

Figure 8: Toddy tapper EBSD map. (a) Large area map showing weak carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is predominantly vertical in all images, with some in the z-axis (out of the page). (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase based on 348 × 244 μm mapping area.

The sword blades investigated here both contain carbide bands that display particle clusters having similar crystallographic orientations. This can be seen on a large scale by viewing the color groupings in a Euler angle map in which the clusters are spread in bands on the long axis of the blade, thereby forming the characteristic long-range carbide bands of warm-worked wootz microstructures (Figure 6a and Figure 7a). These bands regularly intersect the blade surface at shallow angles and are thought to be the origin of the well-known patterning. The orientation clustering behavior is highlighted by examining a subset of a typical carbide cluster (Figures 6b and 6c, Figures 7b and 7c). The other artifact is a tool with a different use and a different microstructure (Figure 8a). The carbide banding in this tool has a significantly weaker texture than the sword blades, as shown by the low mean uniform density value (MUD) in a [010] pole figure. The weaker texture is assumed to be in part due to the lower forging reduction and possibly due to higher temperature forging; however, orientation clustering is still visible.

In addition to orientation clustering characterization, bulk texture data from the carbides were analyzed and used to confirm the predominant deformation direction during forging. Although this direction is known to be edge-wise hammering for the wootz ingot used to fabricate the swords (Figures 9a and 9b), the forming direction for the toddy tapper is not known (Figure 9c). Orthorhombic cube [010] textures were observed in all three artifacts parallel to the hammering direction during forging. Swords 1 and 2 measured high MUD values, 12.3 and 14.3 respectively (Figures 6d and Figure 7d). The toddy tapper displayed a significantly weaker [010] texture of 4.5 (Figure 8d). However, it is sufficient to infer that the principle-forging axis is on the axis shown in Figure 10. The tapper is likely to have experienced two directions of forging, and this has apparently weakened the texture.

Figure 9: Texture indicates predominant deformation direction as shown: (a) for swords, (b) sword blade 1, and (c) the toddy tapper tool (side and top views).

Figure 10: Predominant toddy tapper forming axis based on texture data.

In addition to the carbide orientations, the ferrite matrix was also analyzed for evidence of texture. The bulk texture of the ferrite is shown in terms of {001}, {110}, and {111} pole figures in Figure 11. The texture is weak. No significant difference is evident in the texture of the blade face or cross section. No systematic local grouping of orientations of ferrite was apparent.

Figure 11: Crystallographic textures of the ferrite matrix for the same sample area as the carbide analysis for (a) toddy tapper, (b) blade 1, and (c) blade 2. Suggested forging direction is along the Y-axis in all pole figures.

The data from the two sword blades strongly support the hypothesis that the clusters of coarse carbides with similar orientations originate from a single proeutectoid cementite plate or crystal that has remained undissolved since casting and fragmented during forging cycles. The toddy tapper implement, while weaker in habit, demonstrates the same principle.

Fine Carbide. Investigation of the three artifacts found clusters of a fine submicron dispersion of cementite with an orientation relationship to neighboring pro-eutectoid cementite on prior austenite grain boundaries (Figure 12). This clustering phenomenon differs from that found in the coarse carbides in that no evidence of fragmentation or rotation can be associated with the orientation grouping. Coupled with the spheroidal nature of these carbides, this suggests that they contain information about the heat treatment cycle used to manufacture the artifacts. The observed crystallographic orientation distribution is consistent with either (1) formation from pearlite by spherodising of pearlite lamellae or (2) by the divorced eutectoid transformation (DET) [Reference Verhoeven and Gibson22], or a combination of both mechanisms as local microstructural variations dictate.

Figure 12: Blade 1 fine carbide (a) large area map showing fine carbide crystal orientation clustering and their relationship to prior austenite grain boundaries, (b) pattern quality inset map showing cementite orientations, (c) cementite orientations within 20° of the orientation of a reference particle within the group. (Black = selected orientation, white = greater than 20° misorientation).

Whichever type of nucleation is occurring, the fine particles are adopting the same crystal orientation as the carbide along the prior austenite grain boundaries. The mechanism by which this can occur is not certain because it is clear that both pearlite and divorced eutectoid are present at different locations in the microstructure, depending on the austenising temperature and the weight percent of carbon. Both of these factors can vary significantly throughout the material because the thickness of the artifact and therefore the rate of heat loss during cooling changes from the cutting edge to the shoulder of the sword (~0.1–3 mm). The thickness variation is even more pronounced in the toddy tapper (~2–20 mm).

If the fine particles originate from pearlite, then the orientation grouping can be explained by considering that the pearlite has grown from the cementite according to the Baryatski relation [Reference Reed-Hill and Abbaschian23]. If the fine particles are forming by the DET mechanism, then their orientation grouping is previously unexplained. Pearlite spherodisation is well documented in steels, whereas the non-bainitic DET reaction is not, though this type of DET transformation is known to be favored by annealing at no more than 50ºC below the A1 in the iron-carbon phase system (Figure 1), which is consistent with experiments by Verhoeven and Gibson [Reference Verhoeven and Gibson22].

A possible explanation for the orientation grouping in this case is that the pearlite is in fact forming at the early stages of forging but undergoes incomplete dissolution on successive reheats such that viable cementite nuclei remain in the microstructure at spacings typically associated with DET (~0.2 μm).

Conclusions

Two types of carbide orientation clustering have been observed in three wootz artifacts. Coarse carbides display an orientation clustering behavior where zones of similar orientation (measured within a 20° spread) occur in bands that are formed during forging. This suggests an as-cast particle origin. It is suggested that this provides a means of probing the forging history. Furthermore, a [010] texture was observed in the carbides, and a random texture was observed in the parent ferrite grains for each artifact, confirming the direction of hammer blows used to forge the items. Although this was known in the swords, it was previously not known for the toddy tapper.

Fine carbides were observed to have an orientation clustering habit in close proximity to prior austenite grain boundaries. Although their origin is unclear, these particles are submicron and therefore more likely to dissolve during forging, thus providing information about the temperature history of the material, in particular the distribution of cementite within the ferrite at the onset of the final cooling cycle.

References

[1]Coze, JL, Journal of History of Science, 38(2) (2003) 117127.Google Scholar
[2]Pearson, G, Phil. Trans. Roy. Soc, 85(A) (1795) 322346.Google Scholar
[3]Yule, H and Hobson-Jobson, Burnell, the Anglo-Indian Dictionary. 1st Edition, ed. 1886.Google Scholar
[4]Srinivasan, S and Ranganathan, S. Wootz Steel: An Advanced Material of the Ancient World. Available from: http://materials.iisc.ernet.in/~wootz/heritage/WOOTZ.htm.Google Scholar
[5]Perttula, J, Scandinavian Journal of Metallurgy, 33 (2004) 9297.CrossRefGoogle Scholar
[6]Sherby, OD, ISIJ International, 39(7) (1999) 637648.CrossRefGoogle Scholar
[7]Verhoeven, JD, Pendray, AH, and Dauksch, WE, JOM, 50(9) (1998) 5864.CrossRefGoogle Scholar
[8]Taleff, EM et al., Materials Characterization, 46 (2001) 1118.CrossRefGoogle Scholar
[9]Perttula, J, Scandinavian Journal of Metallurgy, 30(2) (2001) 6568.CrossRefGoogle Scholar
[10] Pendray, AH, How to make a Damascus blade, in Scientific American, 2001.Google Scholar
[11]Verhoeven, JD, Materials Technology, Steel Research, 73(8) (2002) 356365.Google Scholar
[12]Wadsworth, J, Materials Characterization, 47 (2001) 163165.CrossRefGoogle Scholar
[13]Verhoeven, JD et al., Materials Characterization, 30 (1993) 187200.CrossRefGoogle Scholar
[14]Verhoeven, JD et al., Materials Characterization, 24 (1990) 205227.CrossRefGoogle Scholar
[15]Barnett, MR and Balasubramaniam, R, Indian Journal of History of Science, 42 (2007) 633648.Google Scholar
[16]Peterson, DT et al., Materials Characterization, 24 (1990) 355374.CrossRefGoogle Scholar
[17]Kumar, V, Material and Texture Characterization of Deformed Hypereutectoid (Wootz) Steel, Indian Institute of Technology, Kanpur, 2007.Google Scholar
[18]Sullivan, A, Barnett, M, and Balasubramaniam, R, Microsc. Microanal., 13 (2yes) (2007) 11041105.CrossRefGoogle Scholar
[19]Jeffery, D, Iron Processing, 24 (2004) 1316.Google Scholar
[20]Randle, V and Engler, O, Introduction to texture analysis, macrotexture, microtexture and orientation mapping, Gordon and Breach Science Publishers, Amsterdam, The Netherlands, 2000.CrossRefGoogle Scholar
[21]Bunge, HJ, Texture Analysis in Materials Science, Butterworths, London, 1982.Google Scholar
[22]Verhoeven, JD and Gibson, ED, Metallurgical and Materials Transactions A, 29A (1998) 11811189.CrossRefGoogle Scholar
[23]Reed-Hill, RE and Abbaschian, R, Physical Metallurgy Principles. 3rd Edition, Boston, PWS-KENT Publishing Company, 1991.Google Scholar
Figure 0

Figure 1: The iron-carbon phase diagram showing Wootz as a hypereutectoid steel with carbon content 1.6%, forged from cast ingot at high temperature using multiple cycles.

Figure 1

Table 1: Wootz artifact descriptions. Note that all items are hypereutectoid steels.

Figure 2

Figure 2: (a) Electron Backscatter Diffraction (EBSD) system schematic, (b) Kikuchi pattern [20].

Figure 3

Figure 3: The three Euler angles: (ϕ1, Φ, ϕ2) represent the following (ordered) set of rotations, which are defined here. (1) A rotation of ϕ1 about the z-axis followed by, (2) a rotation of Φ about the rotated x-axis (u) followed by, (3) a rotation of ϕ2 about the rotated z-axis (z′).

Figure 4

Figure 4: (a) ⟨100⟩ pole figure construction depicting the cubic unit cell at an arbitrary orientation relative to the sample. The sample surface is parallel to the equatorial plane. (b) The resulting pole figure (stereographic projection of the poles 1, 2, and 3).

Figure 5

Figure 5: EBSD mapping regions indicated in red on the schematics for each artifact: (a) toddy tapper and (b) blades 1 and 2 with z ∥ [010] axis. The dotted lines in (b) show where inhomogeneous material was removed prior to analysis.

Figure 6

Figure 6: Sword 1 EBSD data. (a) Large area map showing carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is vertical in all images. (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase based on 347 × 241 μm mapping area.

Figure 7

Figure 7: Sword 2 EBSD map. (a) Large area map showing carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is vertical in all images. (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase, based on 347 × 259 μm mapping area.

Figure 8

Figure 8: Toddy tapper EBSD map. (a) Large area map showing weak carbide banding and crystal orientation, (b) pattern quality inset map showing cementite orientations among ferrite grains, (c) cementite orientations within 20° of the orientation of a reference particle within the group. Suggested forging direction is predominantly vertical in all images, with some in the z-axis (out of the page). (Black = selected orientation, white = greater than 20° misorientation). (d) Long-range texture of the carbide phase based on 348 × 244 μm mapping area.

Figure 9

Figure 9: Texture indicates predominant deformation direction as shown: (a) for swords, (b) sword blade 1, and (c) the toddy tapper tool (side and top views).

Figure 10

Figure 10: Predominant toddy tapper forming axis based on texture data.

Figure 11

Figure 11: Crystallographic textures of the ferrite matrix for the same sample area as the carbide analysis for (a) toddy tapper, (b) blade 1, and (c) blade 2. Suggested forging direction is along the Y-axis in all pole figures.

Figure 12

Figure 12: Blade 1 fine carbide (a) large area map showing fine carbide crystal orientation clustering and their relationship to prior austenite grain boundaries, (b) pattern quality inset map showing cementite orientations, (c) cementite orientations within 20° of the orientation of a reference particle within the group. (Black = selected orientation, white = greater than 20° misorientation).