Hostname: page-component-586b7cd67f-rdxmf Total loading time: 0 Render date: 2024-11-27T02:01:10.317Z Has data issue: false hasContentIssue false

High Quality Hydrothermal ZnO Crystals

Published online by Cambridge University Press:  13 June 2014

M. Suscavage
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
M. Harris
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
D. Bliss
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
P. Yip
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
S.-Q. Wang
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
D. Schwall
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
L. Bouthillette
Affiliation:
Air Force Research Laboratory, Sensors Directorate, Hanscom AFB, MA 01731, U.S.A.
J. Bailey
Affiliation:
Solid State Scientific Corporation, Hollis, NH 03049, U.S.A.
M. Callahan
Affiliation:
Solid State Scientific Corporation, Hollis, NH 03049, U.S.A.
D. C. Look
Affiliation:
University Research Center, Wright State University, Dayton OH 45435, U.S.A.
D. C. Reynolds
Affiliation:
University Research Center, Wright State University, Dayton OH 45435, U.S.A.
R. L. Jones
Affiliation:
Air Force Research Laboratory, Materials and Manufacturing Directorate, Wright-Patterson AFB, OH 45433, U.S.A.
C. W. Litton
Affiliation:
Air Force Research Laboratory, Materials and Manufacturing Directorate, Wright-Patterson AFB, OH 45433, U.S.A.

Abstract

Zinc Oxide crystals have historically been grown in hydrothermal autoclaves with a basic mineralizer; however, doubts have been raised about the quality of such crystals because they have often exhibited large x-ray rocking curve widths and low photoluminescence (PL) yield with large linewidths. Several ZnO crystals were grown hydrothermally and sliced parallel to the c-plane. This resulted in opposite surfaces (the C+ and C) exhibiting pronounced chemical and mechanical differences. Different surface treatments were investigated and compared by PL both at room temperature and liquid helium temperatures, and by double axis X-ray rocking curve measurements. The high quality of hydrothermally-grown ZnO is substantiated by the narrow rocking curve widths and sharp PL peaks obtained. A critical factor in obtaining these results was found to be surface preparation.

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society

Introduction

Zinc oxide is a wide band-gap semiconductor (3.37eV) Reference Bagnall, Chen, Zhu, Yao, Shen and Goto 1 with potential for applications as emitter devices in the blue to ultraviolet region and as a substrate material for GaN based devices. Because of its high vapor pressure, growth of ZnO from the melt is difficult, and growth by vapor deposition is difficult to control. Hydrothermally grown ZnO has been used previouslyReference Monchamp 2 for surface acoustic wave devices, which do not need the high quality surface that optical or semiconductor device applications require. Therefore, we have performed an initial study of surface preparation and subsequent characterization on hydrothermally grown ZnO in order to produce surfaces suitable for epitaxy.

Experimental

Hydrothermal autoclaves made of high strength steel were used for crystal growth. Because of the high normality of the mineralizing solution, a sealed platinum liner (see reference 2 for an example) was used to isolate the crystal growth environment from the walls of the autoclave.Reference Monchamp 2 The mineralizer solution was a mixture of Li2CO3 , 4 N KOH, and 4 N NaOH, with the fill quantity at 80%. The nutrient was prepared from 99.99% ZnO (Alfa Aesar) powder having particle size < 3 μm, which was sintered for 4 hrs in air at 1350°C in a platinum crucible. The seeds were (0001) plates of ZnO from previous hydrothermal growth runs. During growth, the nutrient zone was at 355°C with a temperature gradient of 10°C declining towards the seed zone. Growth rates in the [0001] directions on the basal seed plates averaged 10 mils per day for the 30 day runs, but growth was anisotropic: the ratio of growth rates between the fast (C+) and slow (C) growth directions was 3 to 1.

Wafers were sliced and the C+ and C planes were identified by etching in nitric acid, following the method developed by Mariano and Hanneman.Reference Mariano and Hanneman 3 Surface properties were analyzed by : double axis x-ray rocking curve with a high resolution four circle x-ray diffractometer; room temperature PL with a 0.25m grating monochrometer, ccd detector, and a 275nm, 5ns pulsed variable wavelength laser source; PL at 4 K with a 1.26m grating spectrometer and at 2.1 K with a high resolution 4.0m grating spectrometer, both equipped with an RCA C31034A photomultiplier and employing a HeCd laser.

For this study, two different surface conditions or surface treatments were studied: a mechanical polish provided by a commercial service, and a chemomechanical polish performed by Eagle-Picher Corporation. We also compared our hydrothermal ZnO (grown at AFRL/Hanscom) to vapor-phase grown ZnO provided by Eagle-Picher. For this comparison, low temperature PL was used to evaluate the presence or absence of excitonic peaks.

Results and Discussion

The crystal growth characteristics of hydrothermal ZnO are dictated by anisotropy between the two opposite surfaces of the basal plane. The opposite sides of a basal plane wafer have different atomic arrangements at their surfaces due to this anisotropy. That is, the C+ side comprises a Zn-rich layer, and the C side comprises an O-rich layer. The resulting electronic charge distribution is illustrated in Fig. 1, adapted from the work of Mariano and Hanneman.Reference Mariano and Hanneman 3

Figure 1. Electronic Charge Distribution of Zinc Oxide.

Typically, seeds were slices cut parallel to the basal plane to maximize the yield of (0001) wafers. The growth habit of hydrothermal ZnO crystals grown on basal plane seeds is shown in Fig. 2.Reference Croxall and Ward 4 For crystal growth in the [0001] direction or C+ sector, the growth rate was faster and the crystal color is clear to light yellow-green. For the {000

} direction or C sector, the growth rate was about 1/3 as fast and the color is typically dark green. Slices were cut as shown from the light green and dark green sectors to distinguish between their chemical and electronic properties. Because of the different growth rates, we speculate that the different colors are due to a difference in impurity incorporation between the two sectors.

Figure 2. Growth habit of hydrothermal Zinc Oxide.

Trace analysis by glow discharge mass spectrometry (GDMS) revealed a slight difference in impurity concentration between the two sectors. The dark sector contains 3-5 ppm of iron, about twice as much as the light sector. This result is similar to other reports on ZnO. 4 The light sector contains 5-6 ppm each of aluminum and silicon, twice as much as the dark sector. Analysis of the free electron concentration by temperature dependent Hall effect revealed further differences. The dark green sector had a low resistivity, with a free carrier concentration of 3×1018 cm−3 at room temperature. The light green sector showed high resistivity, with room temperature electron concentration of 2×1012 cm−3 and mobility of ∼175 cm2/V-sec. From a fit of n vs.1/T, it was determined that the dominant donor in this sector is 0.34 eV below the conduction band, and that donor and acceptor concentrations were about 7×1015 and 1×1015 cm−3, respectively. Thus, the purity in this sector is quite high.

One possible explanation accounting for the chemical and electrical data could entail growth-rate dependent incorporation of impurities or native defects. Differential segregation of impurities may contribute to the chemical and electronic differences between the two sectors, but there is no evidence that dopants like silicon or aluminum could be responsible for the deep level defect. Nor is there any evidence that iron could account for the shallow donor in the dark sector. Another possible explanation is that stoichiometric defects, complexed with impurities, act as compensation centers in the light sector, reducing the free-carrier optical absorption.

Each slice cut parallel to the C-plane has both a Zn-side and an O-side. Both sides of the wafers were polished in the same manner to determine the mechanical and optical properties of the two surfaces. The two surfaces have different chemical reactivities and mechanical properties as a result of surface anisotropy, so that given the same surface treatment, each side shows different results. This is illustrated in Table I which shows the rocking curve half-widths and PL intensities for two different polishing methods. The x-ray rocking curve measures strain in the sub-surface region, where Cu Kα radiation at 1.54 Å has a penetration depth of about 2 microns. A dramatic reduction by a factor of two is seen in the rocking curve width after the combined chemical-mechanical polish. A similar result is seen in the PL intensity at room temperature. At the excitation wavelength of 275 nm the absorption coefficient of ZnO is very high, and therefore the probe depth is on the order of a few nanometers. Thus PL is a very good indicator of surface quality. A comparison of PL intensities indicates the surface is much less damaged by chemical polishing than by mechanical polishing.

Table I. Effect of different surface treatments on hydrothermal ZnO

Surface Preparation Description Mechanical polish Eagle Picher polish
Crystal faces C+ C C+ C
X-ray rocking curve FWHM (arc-sec) 108 104 43 37
3.28 eV PL relative intensity at room temp 0.04 0.5 1.1 1.5

Photoluminescence measurements at room temperature are useful for comparing the quality of ZnO samples. Because of the large exciton binding energy of 60 meV, exitonic emission will survive well above room temperature.1 Thus, the measurement is an indicator for possible stimulated emission and lasing from ZnO at room temperature. Under pulsed excitation at 275 nm, the emission peak position is close to the expected energy of the free exciton. The bandgap of ZnO at room temperature is 3.37 eV, 1 and the observed PL emission peak is at 3.28eV. A comparison of the PL emission spectra for the same ZnO wafer after the two different surface treatments is shown in Figure 3.

Figure 3. Room Temperature PL comparing different polishes.

Low temperature PL measurements give additional information on the fine structure of the emission. Photoluminescence (at 2.1 K) is clearly observed in the intrinsic spectral region from hydrothermally grown ZnO samples. Emission from both the ground state and excited states of the free exciton is shown in Fig. 4. The ground state emission is shown in both the absence (solid line) and presence (dashed line) of an applied magnetic field. The ground state consists of a Γ5 allowed exciton (3.3758eV), and a Γ6 forbidden exciton (3.3740eV) which is allowed in the presence of an applied magnetic field. Observation of both the Γ5 and Γ6 excitons is characteristic of good quality material.

Figure 4. PL Emission of hydrothermal zinc oxide sample.

The observation of excited states of the ground state excitons is even more indicative of high quality material. The n= 2 states of the Γ5 and Γ6 excitons associated with a valence band are not resolved, and occur at 3.4214eV. The n= 3 states of these excitons are resolved and occur at 3.4295eV for the Γ5 exciton and at 3.4280eV for the Γ6 exciton. The selection rules are relaxed for the excited state transitions. From the emission spectra, the exciton binding energies can be obtained assuming the excited states are hydrogenic. The n= 2 state of the exciton associated with the B-valence band is observed at 3.4318eV. The ground state B-exciton (not shown) occurs at 3.3885eV. These data demonstrate that high quality ZnO can be grown by the hydrothermal technique.

The PL spectra in Fig. 5 compare hydrothermal ZnO grown at AFRL Hanscom with vaporphase grown ZnO provided by Eagle-Picher.

Figure 5. Photoluminescence (at 4.2 K) comparing hydrothermal ZnO and vapor-phase grown ZnO.

Photoluminescence of both Hanscom’s hydrothermal and Eagle-Picher’s (E-P) vaportransport grown ZnO crystals (at 4.2 K) is most intense in the near-band-edge energy region, as shown in Figure 5. Spectra have been slightly shifted in energy to facilitate direct comparisons. This figure is for the PL from oxygen face. All the sharp transitions are emissions from the decay of an exciton bound to a complex of a neutral donor and some unknown impurity or defect (X, D ° complex). A comparison of the FWHM and intensity for the two samples with the same surface preparation (E-P polish) but different growth methods shows nearly identical material quality . A comparison of PL spectra for the same Hanscom crystal before and after E-P polish demonstrates the importance of surface preparation. PL from this sample after E-P polish (square markers) is sharper and eight times stronger than before E-P polish (triangle markers). The energy positions of lines this sharp are subject to strain and other point-to-point variations.

The high quality of both Hanscom’s hydrothermal and E-P’s vapor-transport ZnO crystals is again indicated by the sharp PL (not shown) from the zinc face of the two samples (at 4.2 K) which have received E-P’s polish. For the zinc face, the comparison of PL spectra from the same Hanscom sample before and after E-P polish is even more striking than from the oxygen face: PL from the hydrothermal sample before the E-P polish was much broader and three orders of magnitude less intense.

Conclusions:

High quality, bulk ZnO was grown hydrothermally. The high quality of the crystals in this study was demostrated by narrow x-ray rocking curves and sharp PL peaks. The crystal color is non-uniform because of its anisotropic crystal growth habit in which the growth rate of each sector depends on orientation. Slices cut from the lighter region are semi-insulating, whereas those from the dark sector are n-type conducting. Anisotropy is also seen in surface quality of polished slices. For slices cut and polished on both sides of the basal plane, the oxygen face yields sharper and more intense room temperature PL peaks, and a narrower x-ray rocking curve. Improved polishing methods result in significantly improved surface quality as measured by the PL and rocking curve widths. When properly polished, hydrothermal ZnO exhibits optical properties similar to vapor phase grown ZnO. Therefore, proper surface preparation is necessary to evaluate the quality of ZnO substrates. For epitaxy, e.g. of GaN, special care is required to insure that ZnO surfaces are of high quality.

Acknowledgments

This work was funded in part by Air Force Office of Scientific Research.

Footnotes

MRS Internet J. Nitride Semicond. Res. 4S1, G3.40(1999)

References

Bagnall, D. M., Chen, Y. F., Zhu, Z., Yao, T., Shen, M. Y., and Goto, T., Appl. Phys. Lett. 73 (1998) 1038.Google Scholar
Monchamp, R. R., “Growth of Zinc Oxide Crystals – Interim Engineering Progress Report,” Airtron Division of Litton Industries, Morris Plains, New Jersey, ASD project Nr.-7-988, Contract No. AF33(657)-8795, November, 1964.Google Scholar
Mariano, A. N. and Hanneman, R. E., J. Appl. Phys. 34 (1963) 384.Google Scholar
Croxall, D. F. and Ward, R., J. Cryst. Growth, 22 (1974) 117.Google Scholar
Figure 0

Figure 1. Electronic Charge Distribution of Zinc Oxide.

Figure 1

Figure 2. Growth habit of hydrothermal Zinc Oxide.

Figure 2

Table I. Effect of different surface treatments on hydrothermal ZnO

Figure 3

Figure 3. Room Temperature PL comparing different polishes.

Figure 4

Figure 4. PL Emission of hydrothermal zinc oxide sample.

Figure 5

Figure 5. Photoluminescence (at 4.2 K) comparing hydrothermal ZnO and vapor-phase grown ZnO.